Purifying?agent?for?molten?zinc?in?HDG
Name:
Purifying?agent?for?molten?zinc?in?HDG
  • Model:
  • Uses:
  •  
Details

In the light of the high iron and impurity contents in molten zinc, poor fluidness and particles and fold on workpiece often occurred in hot galvanizing plants, our company has organized the famous specialists and scientific and technological personnel in many disciplines at home developed XY-XG-3 type purifying agent for molten zinc, a high and new technical product. It has effectively solved the difficult problem and filled in the gap in this field at home. Through testing and using, the agent reached the anticipated results and is well received by customers. At present the product is applying for a patent. 
Notice
Do well pretreatment work, do not carry the harmful impurity into zinc pot, galvanizing agent needs the acid and iron eliminating, and it would be best if rinsing water for pretreatment could be fluid.
Because of the high volatility of the agent, No.2 operation should be quickly performed.
In order to avoid the splashing of molten zinc causing danger, operators should be well dressed in labor protection articles. Operation with caution and safety first.
Purifying Treatment Method of Molten Zinc:
Keep furnace temperature at 450℃-470℃.
Place dry thermal insulation bricks (with strong water absorption) into box with holes, quickly pour the purifying agent to them, insert the box into molten zinc and move it back and forth until boiling ends, and take out the box with holes.
Eliminate suspended substances on the surface of molten zinc; scatter ammonium chloride (1-1.5 kg/ m2) to further eliminate impurity on the surface.
Repeat the abovementioned steps three or four times.
Add the alloy, which is 0.5% of molten zinc, in uniform distribution way. After all the melting, repeat the abovementioned step once. (If there are excessive aluminum or other alloys in original molten zinc, the step-by-step method can be used)
The temperature is controlled at 430℃-440℃ and the standing time is 6-12 h (time is as long as possible).
When small workpiece is tested (the temperature is at 430℃ and dipping time is not changed), the surface and coating thickness is measured. If the coating is thick, the alloy, which is 0.1 % of molten zinc, can be added. 
The zinc and the alloy can be added at one time until the alloy content in molten zinc reaches 1.5%.
After alloying is completed, the working temperature of molten zinc should be controlled at 440℃±5℃ and the lifting speed of traveling crane at 1.5 m / min.
 

 

返回頂部 電話
主站蜘蛛池模板: 可爱男生被触手入侵下面| 国产精品女在线观看| 伊人久久国产精品| 色播影院性播免费看| 国产黑色丝袜在线观看下| 久久人妻少妇嫩草av蜜桃| 狠狠躁日日躁夜夜躁2022麻豆| 国产成人亚洲综合欧美一部 | 国产一区视频在线免费观看| 97无码免费人妻超级碰碰夜夜| 日韩av无码成人精品国产| 亚洲中文字幕无码日韩| 福利一区二区三区视频在线观看| 国产成人精品无码片区在线观看| igao为爱寻找刺激| 日本牲交大片无遮挡| 亚洲av无码一区二区二三区| 欧美日韩视频一区三区二区| 唐人电影社欧美一区二区| 蜜桃成熟时仙子| 国产精品亚洲欧美一级久久精品 | 在线观看国产成人av片| 久久中文娱乐网| 欧美在线观看视频网站| 可播放的欧美男男videos| 被公侵犯肉体中文字幕| 国产在线jyzzjyzz免费麻豆| 99久久99久久精品国产片| 日本19禁啪啪无遮挡免费动图 | 久久九九国产精品怡红院| 欧美精品在线观看| 又大又湿又紧又大爽a视频| 97国产在线播放| 在线中文字日产幕| aa级国产女人毛片水真多| 日本一区视频在线| 亚洲一级片在线播放| 欧美在线视频导航| 免费不卡在线观看av| 调教女m视频免费区| 国产精品久久久久久久久久影院|